Isotropic polycrystalline BaFe12O19 films with thicknesses of 19, 20, 39, 41 and 485 μm were obtained by slip casting on Al2O3 substrates in three process modes. The crystal structure, surface quality and magnetic hysteresis loop parameters of the specimens were studied using X-ray diffraction, optical microscopy and vibromagnetometry. The quality and properties of the as-synthesized specimens and those grown in different process modes were studied. Films grown in Mode 2 proved to have the highest magnetic parameters and surface quality. The specific saturation magnetization of these films was σs = 73÷76 emu/g, the magnetization coercive force was IHc = 3.07÷3.08 kOe and the magnetic texture degree was f = 11.82÷15.76%.